Cu-converter slag
Fe: 52%
Cu: 2.6%
Zn: 0.43%
Co: 0.36%
Ni: 0.05%
Roasting agent: Fe
2
(SO
4
)
3
× H
2
O
Fe
2
(SO
4
)
3
× H
2
O /slag ratio: 1
Roasting T: 300 – 800°C
Roasting time: 0.5 – 4 h
Extractant: H
2
O and H
2
SO
4
FS: < 74µm
L/S: 5 (20% of solid)
T: 25°C
LT: 0.5 h
AS: present (n.i. rpm)
Metals recovery increases with increased roasting temperature to 500-550°C
reaching Cu> 95% (24.7 g/kg) #, Zn 65% (2.8 g/kg), Co 40% (1.4 g/kg), Ni<
15% (0.08 g/kg) (0.5 h leaching)
Roasting time of 2 h was found to give the best values of extracted metals
during 0.5 h leaching
Increase of ferric sulfate/slag ratio improves Cu extraction (Cu~75% (~19.5
g/kg) at 0.5 ratio, Cu> 95% (24.7 g/kg) # at 1-2.5 ratio
Altundoǧan
and Tümen
(1997)
Do'stlaringiz bilan baham: |